Almost every gear that works for a living is surface hardened, and the reason is a compromise that runs through all of machine design: the tooth flank wants to be hard, to resist wear and pitting, while the tooth core and the blank want to stay tough, to absorb bending and shock without cracking. Through-hardening a gear all the way through gives you a hard but brittle component, and leaving it soft gives you a component that wears out quickly, so the engineering answer is a hard case on a tough core, produced by one of three families of surface hardening: case carburizing, nitriding and induction hardening. Choosing between them is one of the first decisions in any custom gear order, because the choice sets the steel grade, the machine schedule, the distortion the gear will show, the grinding allowance and the price. The three processes are not interchangeable, and the right answer depends on the load, the speed, the size of the gear, the accuracy it must hold and the quantity you need. This guide compares the three routes on the dimensions that actually decide an order, and ends with the selection logic the shop uses when the application is described.
Case carburizing is the workhorse of heavy-duty gear manufacture, and it starts from low-carbon steels such as 20CrMnTi, 16MnCr5 and 20CrMnMo, which are soft enough to machine in the soft state and then enriched with carbon at the surface. The parts are heated in a carbon-rich atmosphere, usually gas carburizing, for many hours, so that carbon diffuses into the surface to a controlled depth, typically 0.6 to 1.5 mm for automotive and industrial gears and deeper, up to 3 mm or more, for large heavy-duty gears. The parts are then quenched and tempered, which leaves a hard, high-carbon case with a typical surface hardness of 58 to 62 HRC and a tough, low-carbon core. Carburizing wins where the duty is severe: high contact stress, shock loads, reversing torque and big bending moments, which is why automotive transmission gears, differential gears, industrial reducers and heavy machinery pinions are carburized. The price of the process is distortion: the long thermal cycle and the quench move the geometry, so carburized gears that must hold a high accuracy grade are ground after hardening, which adds a machining step and cost. Carburized gears also need the case to be controlled carefully, because an over-carburized case is brittle and an under-carburized one wears early.
Nitriding is the quiet alternative that many engineers under-use. Instead of adding carbon, it adds nitrogen to the surface of an already hardened steel, usually a nitriding grade such as 38CrMoAl or a medium-carbon alloy steel, at a comparatively low temperature, around 500 to 550 degrees Celsius, for tens of hours. Because the process runs below the transformation temperature of the steel, distortion is minimal, the part keeps the accuracy it was machined to, and no re-grinding is needed after treatment in most cases, which makes nitriding attractive for finished gears, precision splines and parts whose geometry is hard to grind. The surface hardness is higher than carburizing, typically 60 to 68 HRC equivalent, with excellent wear resistance and good resistance to scuffing, and the thin, hard, brittle case, usually 0.2 to 0.6 mm, is well suited to light to moderate loads, continuous running and applications where dimensional stability matters more than impact resistance. The limits are the inverse of the strengths: the thin case cannot carry heavy shock or high contact stress, the long cycle time at temperature is not cheap for large batches, and nitriding does not improve the core, so the steel must already be strong enough in the soft state.
Induction hardening is the fast, local option, and it treats the tooth flanks, or the whole toothed region, by heating the surface with a high-frequency alternating field and quenching it immediately. It works on medium-carbon steels such as 45, 40Cr and 42CrMo, which already carry enough carbon to harden on quenching, and it can be applied selectively, hardening only the tooth surfaces while leaving the bore, the keyway and the rest of the blank soft, which is exactly what many shafts and gear teeth need. The case depth can be tuned from a fraction of a millimetre to several millimetres, surface hardness runs 50 to 58 HRC for medium-carbon steels, and the cycle is short, so it is the cheapest of the three routes for medium-size gears and shafts produced in quantity. The trade-offs are distortion, which depends on how evenly the inductor heats the part, the need for accurate coil design for each geometry, and the hardness ceiling, which is lower than carburizing or nitriding because the steel does not gain carbon or nitrogen, only a hardened martensitic case from the carbon it already has. Induction hardening is the standard answer for moderate-load gears, shafts with integral gears, and parts where a selective hardened zone saves money.
Set side by side, the three processes line up predictably. On achievable surface hardness, nitriding leads at 60 to 68 HRC equivalent, carburizing follows at 58 to 62 HRC, and induction trails at 50 to 58 HRC on plain medium-carbon steels. On case depth, carburizing offers the deepest and most controllable cases, induction covers a wide middle range that can be tuned locally, and nitriding produces the thinnest case, which is fine for wear but not for heavy shock. On distortion and accuracy, nitriding is best because the low process temperature barely moves the part, induction is moderate and geometry-dependent, and carburizing distorts the most, so high-grade carburized gears must be ground afterwards. On cost for a typical medium-size gear, induction is cheapest when it suits the duty, carburizing plus grinding is the premium route for heavy duty, and nitriding sits between them, with the long cycle time penalising big batches. On materials, carburizing needs low-carbon case-hardening steels, nitriding needs nitriding grades or pre-hardened alloy steels, and induction needs medium-carbon steels with enough carbon to harden. On typical applications, carburized gears dominate vehicles and heavy industry, nitrided gears suit precision instruments, machine spindles, servo drives and large gears that must stay accurate, and induction-hardened gears and shafts suit moderate industrial duty in quantity.
The selection logic a gear shop actually uses starts from the duty, not from a favourite process. If the gear must carry heavy shock, high contact stress or reversing load, and accuracy can be restored by grinding, carburizing is the default, with the steel grade chosen from the case depth required and the core toughness needed. If the gear must hold tight accuracy without re-grinding, runs at moderate load, or is too large or too thin-walled to grind after hardening, nitriding is the answer, with the steel chosen to be nitridable and strong enough in the core. If the gear is a moderate-load production part or an integral-gear shaft, and cost per piece matters, induction hardening is worth quoting, with the case depth tuned to the tooth size so that the hardened case does not spall at the tooth root. When the duty is marginal between two routes, the deciding factors are the quantity, because induction amortises its tooling cost across a run, and the accuracy grade, because a grade that forces post-hardening grinding pushes the decision toward carburizing, where grinding is expected, or nitriding, where it is avoided. Whatever the route, the customer should leave the order with three numbers on the inspection sheet: the surface hardness, the case depth and the core hardness, because those three values, matched against the duty, are what the gear will actually live and die by.